Strain rate and oxidation effects on crack initiation at 600 and 650 °C in a nickel-based superalloy

N/A
N/A
Protected

Academic year: 2021

Partager "Strain rate and oxidation effects on crack initiation at 600 and 650 °C in a nickel-based superalloy"

Copied!
8
0
0

Texte intégral

(1)

O

pen

A

rchive

T

OULOUSE

A

rchive

O

uverte (

OATAO

)

OATAO is an open access repository that collects the work of Toulouse researchers and

makes it freely available over the web where possible.

This is an author-deposited version published in :

http://oatao.univ-toulouse.fr/

Eprints ID : 19781

To link to this article : DOI:10.1080/09603409.2016.1169665

URL :

http://dx.doi.org/10.1080/09603409.2016.1169665

To cite this version :

Perrais, Maxime and Seror, Alexandre and

Burteau, A. and Andrieu, Eric and Poquillon, Dominique Strain rate

and oxidation effects on crack initiation at 600 and 650 °C in a

nickel-based superalloy. (2016) Materials at High Temperatures,

vol. 33 (n° 3). pp. 241-247. ISSN 0960-3409

Any correspondence concerning this service should be sent to the repository

administrator:

[email protected]

(2)

Strain rate and oxidation effects on crack

initiation at 600 and 650 °C in a nickel-based

superalloy

M. Perrais

1,2

, A. Seror

2

, A. Burteau

3

, E. Andrieu

1

and D. Poquillon

1

 

Nickel-based superalloys are sensitive to an oxidation-assisted intergranular crack (OAIC) growth

mechanism. Crack initiation during slow strain rate tensile tests is investigated at 600 and 650 °C, at

different strain rates, with or without oxidation on a direct-aged material. A V-shaped sample geometry

is used to promote damage initiation for a specific stress triaxiality. The critical mechanical loading paths

inducing intergranular crack initiation as well as the effect of oxidation are discussed.

Keywords: Ni-based superalloys, Direct aged alloy 718, Oxidation, Environment assisted cracking

Introduction

Alloy 718 is a nickel-based superalloy used for a wide range RI DSSOLFDWLRQV LQ ¿HOGV LQFOXGLQJ DHURVSDFH FKHPLFDO DQG QXFOHDUHQJLQHHULQJ0DQ\VWXGLHVKDYHEHHQGHYRWHGWRLWV PHFKDQLFDOEHKDYLRXUGXULQJIDWLJXHWHVWV1–4 creep tests5–7 and creep- fatigue tests.8–12+RZHYHUPRVWRIWKHPKDYHIRFXVHGRQ standard solution-treated and aged condition 718 alloys (STD   ZKRVH PLFURVWUXFWXUH1012 GLIIHUV IURP WKH GLUHFWDJHG PDWHULDO '$ 7KLVVWXG\LVGHYRWHGWR'$XVHGLQ ORZSUHVVXUHWXUELQHGLVFVRIDLUFUDIWHQJLQHV7KHHOHYDWHGWHP-SHUDWXUHIDWLJXHFUDFNJURZWKEHKDYLRXULQ67'GHSHQGV RQWKHHQYLURQPHQWDQGOLNHPDQ\RWKHUQLFNHOEDVHGVXSHU-DOOR\VLVVHQVLWLYHWRR[LGDWLRQDVVLVWHGLQWHUJUDQXODUFUDFNLQJ (OAIC).±+RZHYHUIHZHUVWXGLHVDUHGHYRWHGWR$OOR\ IRUWHPSHUDWXUHVDERYHƒ&EXWVRPHSDSHUVKRZHGWKDW WKHDOOR\LVVHQVLWLYHWRLQWHUJUDQXODUFUDFNLQJDWƒ&17 0HFKDQLFDOWHVWLQJVKRZVWKDW'$H[KLELWVDKLJKHU WHQVLOHVWUHQJWKWKDQ67'10,QWKHSUHVHQWZRUNFUDFN initiation in DA 718 during slow strain rate tensile tests is LQYHVWLJDWHGDWDQGƒ&ZLWKRUZLWKRXWR[LGDWLRQ7KH SXUSRVHLVWRFKHFNWKHHIIHFWVRIVWUDLQUDWH GRZQWRí sí) DQGR[LGDWLRQRQGDPDJHLQLWLDWLRQ 7KHFULWLFDOPHFKDQLFDOORDGLQJSDWKVLQGXFLQJLQWHUJUDQX- ODUFUDFNLQLWLDWLRQDUHGHWHUPLQHGYLDDGXDODSSURDFKREVHU-YDWLRQRIFUDFNLQLWLDWLRQORFDWLRQVRQ9VKDSHGVSHFLPHQV (Fig. 1 DQGVXSSRUWLQJ¿QLWHHOHPHQW )( VWUHVVDQGVWUDLQ FDOFXODWLRQV7RDVVHVVWKHUROHRIR[LGDWLRQLQFUDFNIRUPD- WLRQWHVWVZHUHFRQGXFWHGXVLQJHLWKHUDODERUDWRU\DLURUYDF-XXPHQYLURQPHQW)XUWKHUPRUHVRPHSUHR[LGLVHGVDPSOHV ZHUHDOVRWHVWHG0HFKDQLFDOWHVWVZHUHVWRSSHGDWDGLIIHUHQW VWUDLQOHYHOVVXEVHTXHQWO\GDPDJHLQLWLDWLRQVLWHVDQGWKHLU FRUUHVSRQGLQJ RFFXUUHQFH IUHTXHQFLHV ZHUH LGHQWL¿HG DQG UHFRUGHGWKDQNVWRGHWDLOHG6(0REVHUYDWLRQV

,QWKLVDUWLFOHPDWHULDODQGH[SHULPHQWDOSURFHGXUHVDUH ¿UVWGHWDLOHG1H[WWKHUHVXOWVRIWKHPHFKDQLFDOWHVWVDQG 6(0REVHUYDWLRQVDUHSUHVHQWHGDQGGLVFXVVHG

Material and samples

7KHLQYHVWLJDWHGDOOR\ZDVREWDLQHGIURPDGLUHFWDJHG IRUJHGGLVFSURYLGHGE\61(&0$7KHFKHPLFDOFRPSRVL-WLRQRIWKHDOOR\LVSUHVHQWHGLQ7DEOH1. In order to get VDPSOHZLWKWKHJDXJHOHQJWKLQWKHFLUFXPIHUHQWLDOGLUHFWLRQ WKHGLVFZDV¿UVWGLYLGHGLQWRVHFWLRQV7KHVHEORFNVZHUH ¿UVWURXJKO\PDFKLQHGWRREWDLQWUDSH]RLGVHFWLRQVORFDWHGLQ WKHEXONZKHUHWKHPLFURVWUXFWXUHLVKRPRJHQHRXV)LJXUH1 VKRZVDQLOOXVWUDWLRQRIWKLVPLFURVWUXFWXUHFKDUDFWHULVHGE\ URXJKO\HTXLD[HGVPDOOJUDLQV ±ȝP E\JOREXODUįSKDVH DQGE\WKHSUHVHQFHRIRFFDVLRQDOFDUELGHVDQGFDUERQLWULGHV SHUPP2 7KHDYHUDJHVXUIDFHIUDFWLRQRIWKHį

precip-LWDWHVLVEXWWKHGLVWULEXWLRQLVXQHYHQGXHWRIRUJLQJ 7KHSUHFLSLWDWHGLDPHWHUIROORZVDORJQRUPDOGLVWULEXWLRQ DQDYHUDJHGLDPHWHURIȝPDQGDPHGLDQGLDPHWHURI ȝP $FFRUGLQJO\PRVWRIWKHSUHFLSLWDWHV  KDYH DGLDPHWHUVPDOOHUWKDQȝP'XHWRFLUFXODUIRUJLQJFDU-ELGHVDUHRIWHQDOLJQHGLQWKHFLUFXPIHUHQWLDOGLUHFWLRQ$V illustrated on Fig. 1WKHįSKDVHLVORFDOLVHGPDLQO\LQWKH

JUDLQERXQGDULHV,PDJHDQDO\VLVOHGWRDYROXPHIUDFWLRQRI globular įSKDVHRI&ODVVLFDOO\67'LVVROXWLRQ DQQHDOHGDIWHUIRUJLQJ KDWƒ& IROORZHGE\DFRQYHQ-WLRQDODJHLQJKHDWWUHDWPHQW ƒ&KIXUQDFHFRROHGDW ƒ&Kƒ&K )RU'$WKH¿UVWVWHSLVVNLSSHG 7KHUHPDLQLQJįSKDVHSUHYHQWVJUDLQJURZWKGXULQJWKHVHF-RQGVWHSDQGLPSURYHVIDWLJXHSURSHUWLHV,QDGGLWLRQWRWKH intragranular Ȗƍ and ȖƎSUHFLSLWDWHVWKDWDUHDOVRREVHUYHGLQ 67'WKHJUDLQERXQGDULHVRI'$DSSHDUWREHµGHFR-UDWHG¶ZLWKWKLQįSKDVHSUHFLSLWDWHVZKHUHQRJOREXODUįSKDVH SUHFLSLWDWHVDUHREVHUYHG )LJ2 7KLVQDQRį platelets are

QPZLGHDQGFDQUHDFKVHYHUDOKXQGUHGQDQRPHWUHVORQJ 7KLVW\SHRISUHFLSLWDWLRQLVRIWHQREVHUYHGEXWQRWV\VWHP-DWLF)XUWKHUPRUHDSUHFLSLWDWHIUHH]RQH ±QPZLWK LV DOZD\VREVHUYHGDURXQGWKHVHWKLQįSKDVHSUHFLSLWDWHV:KHQ DOOR\LVVXEPLWWHGWRVROXWLRQDQQHDOHGKHDWWUHDWPHQW DIWHUIRUJLQJVXFKSUHFLSLWDWLRQ DQG3)= RQJUDLQERXQGD-ULHVLVQHYHUREVHUYHG7KLVYHU\SDUWLFXODUPLFURVWUXFWXUHRI JUDLQERXQGDULHVLQ'$LVDNH\HOHPHQWIRUXQGHUVWDQG-LQJLQWHUJUDQXODUFUDFNVLQLWLDWLRQ'XULQJVDPSOHSUHSDUDWLRQ SDUWLFXODUFDUHZDVWDNHQQRWWRFKDQJHWKHPLFURVWUXFWXUH especially in surface. DOI 10.1080/09603409.2016.1169665

*Corresponding author, email [email protected]

1CIRIMAT, Université de Toulouse, CNRS, INPT, UPS, 4 allée Emile Monso –

BP 44362 – 31030 TOULOUSE cedex 04, France

2SNECMA – Rond-Point René Ravaud – 77550 Moissy–Cramayel, France 3TURBOMECA – Avenue Joseph Szydlowski 64511 Bordes, France

(3)

$OO WKH VSHFLPHQV ZHUH PDFKLQHG XVLQJ HOHFWULFDO GLV-FKDUJH PDFKLQLQJ %HIRUH EHLQJ REVHUYHG RU WHVWHG WKH VDPSOHVZHUHFDUHIXOO\SROLVKHGWRUHPRYHWKLVKHDWDIIHFWHG ]RQH7KHWKLFNQHVVRIWKH+$=GXHWRWKHPDFKLQLQJSURFHVV DIIHFWLQJWKHDOOR\ZDVȝPDQGZDVGHWHUPLQHGZLWK6(0 DQG7(0REVHUYDWLRQV7KLVOD\HUZDVFDUHIXOO\UHPRYHG WKDQNVWRVXFFHVVLYHSROLVKLQJZLWKVLOLFRQFDUELGHSDSHUV RI GHFUHDVLQJ JULW VL]HV    DQG 3  7KH SXUSRVHZDVWRREWDLQDPLUURUVXUIDFHVWDWHDOORZLQJWKH REVHUYDWLRQ RI FUDFN LQLWLDWLRQ ,Q RUGHU WR HQKDQFH GDP-DJHLQLWLDWLRQ9VKDSHGVSHFLPHQVZHUHXVHG )LJ 7KH 9VKDSHGVSHFLPHQJHRPHWU\SURYLGHVDQDUHDLQWKHLQWUDGRV RIWKH9ZKLFKORFDOLVHVVWUDLQDQGGDPDJH7KLVJHRPHWU\ was initially proposed by Totsuka et al.1819 as it enabled HQKDQFHGVWUHVVLQJRIWKHVDPSOHVXUIDFHDQGKDVSUHYLRXVO\ been used on nickel-based alloys1720 for crack initiation stud- LHV7KLV9VKDSHGVDPSOHJHRPHWU\LVXVHGWRSURPRWHGDP-DJHLQLWLDWLRQIRUDVWUHVVWULD[LDOLW\ GH¿QHGE\WKHUDWLRRI WKHPHDQVWUHVVWRWKHHTXLYDOHQWVWUHVV UHSUHVHQWDWLYHRIUHDO RSHUDWLQJFRQGLWLRQV+RZHYHUDVVWUHVVDQGVWUDLQDUHQRW KRPRJHQRXVLQVXFKVDPSOHWHQVLOHWHVWVDUHWREHFRXSOHG ZLWK¿QLWHHOHPHQW )( DQDO\VLVIRUWHVWGHVLJQDQGGLJLWDO LPDJHFRUUHODWLRQ ',& WRYDOLGDWH7KHIROORZLQJVHFWLRQ ZLOOGHWDLOWKHVHWZRSRLQWV

Experimental procedures

)(FDOFXODWLRQVZHUHSHUIRUPHGWRGHWHUPLQHWKHVFDOHDQG GLVWULEXWLRQRIWKHORFDOVWUHVVDQGVWUDLQWHQVRU¿HOGVVFDOHLQ WKH9VKDSHGVSHFLPHQWKURXJKRXWDWHQVLOHWHVW7KHVH'FDO-FXODWLRQVZHUHSHUIRUPHGXVLQJ=HEXORQ¿QLWHHOHPHQWFRGH21 WRJHWKHUZLWKDQHODVWLFYLVFRSODVWLFLVRWURSLFFRQVWLWXWLYHODZ ZKLFKZDVLGHQWL¿HGE\DVWDQGDUGWHQVLOHWHVW ísí) and UHOD[DWLRQWHVWVRQWKHVWXGLHGPDWHULDO7KHREMHFWLYHRI)( VLPXODWLRQVZDVWZRIROGRQWKHRQHKDQGGHIRUPDWLRQLQWKH DSH[RIWKH9IRUDQLPSRVHGGLVSODFHPHQWRIWKHVSHFLPHQ JULSZDVHYDOXDWHGDQGRQWKHRWKHUKDQGWKHUHVXOWVRIWKH VLPXODWLRQVZLWKWKHGHIRUPDWLRQ¿HOGVREWDLQHGE\',&DUH FRPSDUHG)RUWKLVSXUSRVHWKHSKRWRJUDSKVZHUHWDNHQZLWK D&DQRQ(26'FDPHUDHTXLSSHGZLWKDPDFUROHQVDQGDQ LQWHUYDOWLPHU2QWKHLPDJHVREWDLQHGWKHWKLFNQHVVRIWKH9 PPFI)LJ ZDVGH¿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íPEDU RQDVFUHZGULYHQ076WHVWLQJPDFKLQHDW FRQVWDQWFURVVKHDGYHORFLWLHV7KUHHGLVSODFHPHQWUDWHV  DQGȝPVí ZHUHXVHGWRLPSRVHWKUHHGLIIHUHQWVWUDLQUDWHV 7KHKHDWLQJRIWKHVSHFLPHQZDVVXSSOLHGE\DWKUHH]RQH UDGLDWLYHIXUQDFH7KHWHPSHUDWXUHZDVFRQWUROOHGWKDQNVWR WKUHH.W\SHWKHUPRFRXSOHVVSRWZHOGHGRQWKHVDPSOH8VLQJ WKLVV\VWHPWHPSHUDWXUHJUDGLHQWVZLWKLQWKHVDPSOHVZHUH PDLQWDLQHGEHORZƒ&6DPSOHVZHUHSUHKHDWHGIRURQHKRXU EHIRUHWKHWHVWWRVWDELOLVHWKHVDPSOHDQGJULSVWHPSHUDWXUH 7KHJDXJHOHQJWKRIHDFKWHVWHGVDPSOHZDVH[DPLQHG ZLWK D /(2 93 6(0 HTXLSSHG ZLWK DQ ('6 6\VWHP 3*7,0,; 2EVHUYDWLRQVIRFXVHGRQWKHLQWUDGRVRIWKH9 îPP2DUHD ZKLFKZDVH[SHFWHGWREHWKHSUHIHUHQWLDO DUHDIRUGDPDJHDVVXEPLWWHGWRWHQVLRQ$V\VWHPDWLFVFDQRI WKHDUHDZDVFRQGXFWHGWRORFDWHDQGPHDVXUHWKHOHQJWKRIWKH FUDFNV,PDJHVZHUHPDGHXVLQJERWKVHFRQGDU\HOHFWURQDQG backscattered electrons to identify cracks initiated on carbides RUFDUERQLWULGHV(DFKFUDFNZDVORFDOLVHGDQGPHDVXUHGDQG WKHSUHVHQFHRIDSUHFLSLWDWHQHDUE\LVUHFRUGHG)LJXUH4a LOOXVWUDWHVDFUDFNLQLWLDWHGRQDFDUELGHDQGSURSDJDWHGLQWKH DOOR\ZKHUHDV)LJ4bVKRZVDQLQWHUJUDQXODUFUDFNLPLWDWLRQ 2QO\FUDFNVORQJHUWKDQȝPZHUHPHDVXUHG$VWDWLVWLFDO 10 m Carbides phase

1 Typical microstructure of the alloy of this work. Optical microscopy etched using Kalling’s reagent

Table 1 Chemical composition of 718 alloy (weight %)

Ni Cr Fe Nb (+Ta) Mo Ti Al

50–55 17–21 Bal. 4.75–5.5 2.8–3.3 0.65–1.15 0.2–0.8

phase

PFZ

2 TEM observation of DA 718 grain boundary with thin

ͣ phase on the GB and a precipitate-free zone (PFZ)

(4)

DQDO\VLVRIWKHFROOHFWHGGDWDLQFOXGLQJWKHQXPEHURIFUDFNV SHUPP2DQGWKHIUDFWLRQRIFUDFNVOLQNHGWRDFDUELGHRUD FDUERQLWULGHZDVDOVRGRQH7HVWVZHUHSHUIRUPHGDPLQLPXP RIWZRWLPHVIRUUHSHDWDELOLW\1RVWDWLVWLFVRQWKHGHSWKRIWKH FUDFNVLVDYDLODEOHLQWKHSUHVHQWVWXG\

Results

Finite element simulations

)LQLWHHOHPHQWVLPXODWLRQVKDYHEHHQFDUULHGRXWDWDQG ƒ&DQGDOOWKHH[SHULPHQWDOFRQGLWLRQVKDYHEHHQFDOFX-ODWHG7KHFRUUHVSRQGLQJGLVSODFHPHQWRIWKHVSHFLPHQJULS RUPP ZDVLPSRVHGDWDJLYHQGLVSODFHPHQWUDWH DQGȝPVí )RUHDFKVLPXODWLRQZHREWDLQHGWKH GLVSODFHPHQWYVORDGFXUYH )LJ5 ZKLFKZDVFRPSDUHGZLWK WKHH[SHULPHQWDOGDWDDQGWKHVWUDLQLQWKHDSH[ LQWUDGRV RI WKH9 )LJ ZKLFKZDVFRPSDUHGZLWK',&UHVXOWV*RRG DJUHHPHQWZDVREWDLQHG $Wƒ&LQWKHUDQJHRIFRQGLWLRQVWHVWHGWKHVWUDLQ UDWHGRHVQRWVLJQL¿FDQWO\FKDQJHWKHIRUFHYVGLVSODFHPHQW FXUYH7KHVSHFLPHQRSHQVRXWGXULQJWKHWHVWDQGWKHRSHQLQJ RIWKHOHYHUDUPVZDVOLQNHGWRWKHJHRPHWU\RIWKHVDPSOH 7KHPD[LPXPFXPXODWLYHGHIRUPDWLRQZDVORFDOLVHGLQWKH FHQWUHRIWKH9DQGIRUWKHPD[LPXPHORQJDWLRQRIPP UHDFKHG)RULPSRVHGHORQJDWLRQVRIPPPPDQG PPWKHFDOFXODWHGYDOXHVZHUHDQG7KHSODVWLF ]RQHZDVOLPLWHGWRWKHFHQWUHRIWKH9 )LJ). $Wƒ&VWUDLQUDWHHIIHFWVZHUHQRWLFHDEOHDVLOOXVWUDWHG on Fig. 5 $VIRUWKHVLPXODWLRQDQGWKHH[SHULPHQWWKHGLV-SODFHPHQWZHUHLPSRVHGIRUDJLYHQGLVSODFHPHQWWKHVWUDLQ ¿HOGDWƒ&ZDVYHU\VLPLODUWRWKHRQHDWƒ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¿HOGZDVXVHGWRFDOFXODWHWKHUHIHUHQFH VWUDLQUDWHRIWKHWHVWZKLFKLVWKHVWUDLQUDWHLQWKHWHQVLOH GLUHFWLRQRIWKHSRLQWRIWKHLQWUDGRVORFDWHGLQWKHPLGGOH RIWKHVSHFLPHQ$QLPSRVHGGLVSODFHPHQWUDWHRIȝPVí

corresponded to a reference strain rate of 10í sí9DOXHVRI 10í and 10í síFRUUHVSRQGHGWRDQGȝPVí.

SEM observations of crack initiations

$ JUHDW QXPEHU RI WHVWV   KDYH EHHQ FDUULHG RXW XQGHU GLIIHUHQW FRQGLWLRQV 6(0 REVHUYDWLRQV ZHUH XVHG WR VFDQ

3 Sketch of V-shaped specimens

Crack initiated on a carbide

4a SEM observations examples of crack initiation on carbide. The tensile stress direction is indicated by the white arrow

Intergranular crack

4b SEM observations examples of intergranular crack initiation. The tensile stress direction is indicated by the white arrow

(5)

rates (10í and 10í sí FUDFNLQLWLDWLRQVZHUHOLQNHGWRD SUHFLSLWDWHV FDUELGHVRUFDUERQLWULGHV 7KHWHPSHUDWXUH  RUƒ& RUWKHHQYLURQPHQW DLURUYDFXXP GLGQRWVHHP WRFKDQJHWKHUHVXOWV:KHQWKHFXPXODWLYHVWUDLQH[FHHGHG VRPHLQWHUJUDQXODUFUDFNLQLWLDWLRQVZHUHREVHUYHGDW WKHUHIHUHQFHVWUDLQUDWHRIí síEXWWKH\UHSUHVHQWHGOHVV WKDQRIFUDFNLQLWLDWLRQV +RZHYHUIRUWKHWHVWVFRQGXFWHGDWWKHVORZHVWUHIHUHQFH strain rate (10í sí FUDFNLQLWLDWLRQZDVSUHGRPLQDQWO\LQWHU-JUDQXODUERWKIRUYDFXXPDQGDLUWHVWV )LJ8 DQGWKHVH LQWHUJUDQXODUFUDFNLQLWLDWLRQVZHUHORFDWHGZKHUHFXPXODWLYH VWUDLQZDVODUJHUWKDQ )LJ9 7KXVVORZHUVWUDLQUDWHV SURPRWHGLQWHUJUDQXODUFUDFNLQLWLDWLRQ&UDFNLQLWLDWLRQVZHUH PRVWO\OLQNHGWRFDUELGHVIRUFXPXODWLYHVWUDLQVEHORZ 7HQVLOHWHVWVFDUULHGRXWXQGHUDLUJHQHUDWHGPRUHLQWHUJUDQX-ODUFUDFNDWƒ&WKDQDWƒ& )LJ10 7KHRSSRVLWHWUHQG ZDVREVHUYHGIRUYDFXXPWHVWV&UDFNGHQVLW\ZDVODUJHUE\D IDFWRURIFRPSDUHGWRUHVXOWVREWDLQHGXQGHUDLU ,QRUGHUWREHWWHUXQGHUVWDQGWKHFRXSOLQJHIIHFWGXHWRR[L-GDWLRQDGGLWLRQDOWHVWVZHUHSHUIRUPHG6RPHVDPSOHVZHUH SUHR[LGLVHGDWRUƒ&LQWKHWHQVLOHGHYLFHZLWKRXW ORDGLQJDQGIRUWKHVDPHGXUDWLRQ K DVWKHWHVWGXUDWLRQ RIWKHORQJHVWWHQVLOHWHVWV$IWHUWKHVHKHDWWUHDWPHQWV6(0 REVHUYDWLRQVUHYHDOHGQRFUDFNLQLWLDWLRQLQWKHPDWUL[KRZ-HYHUFDUELGHR[LGDWLRQDQGRUIUDFWXUHVZHUHQRWLFHG7KRVH SUHR[LGLVHGVDPSOHVZHUHWKHQVXEPLWWHGWRVORZVWUDLQUDWH WHQVLOHWHVWVDWWKHVORZHVWUHIHUHQFHVWUDLQUDWH í sí) under GLIIHUHQWFRQGLWLRQV ƒ&±DLUYDFXXP  6XUSULVLQJO\LQWHUJUDQXODUFUDFNLQLWLDWLRQUDWHZDVORZHU IRU SUHR[LGLVHG VDPSOHV )LJ10  $QG IXUWKHUPRUH LW

GHFUHDVHGPRUHIRUWHVWVSHUIRUPHGXQGHUDLU7KHSUHR[L-GDWLRQVHHPVWRLQKLELWLQWHUJUDQXODUFUDFNLQJLQWKH'$ ZKHQVORZVWUDLQUDWHVWHVWVDUHFRQGXFWHGXQGHUDLU,WVHHPV WKDWWKHR[LGDWLRQKDVDEHQH¿FLDOHIIHFWRQWKHLQWHUJUDQXODU FUDFNLQLWLDWLRQRILQWKLVDOOR\

Discussion

6RPHWHQVLOHÀDWVSHFLPHQVZHUHWHVWHGDWORZVWUDLQUDWHWR FRPSDUHGDPDJHVEHWZHHQWKHVHWZRJHRPHWULHV)RUWKHVH VDPSOHVWKHPLQLPXPDFKLHYDEOHVWUDLQUDWHZDVîí sí DQGWKHJDXJHOHQJWKZDVWLPHVODUJHUWKDQWKHRQHRIWKH9 VDPSOHV+RZHYHUDWDQGƒ&QRLQWHUJUDQXODUFUDFN WKHDUHDRILQWHUHVW [PP RQWKHLQWUDGRVRIWKH97KHVH FKDUDFWHUL]DWLRQVUHYHDOHGWKDWWKHODUJHUWKHLPSRVHGFXPXOD-WLYHVWUDLQWKHODUJHUWKHQXPEHURIFUDFNLQLWLDWLRQV )LJ7). )RUWKHWHVWVFRQGXFWHGIRUWKHWZRIDVWHVWUHIHUHQFHVWUDLQ

5 Comparison between experimental data and FE results for force / displacement curves obtained during the opening of the V at 650 °C. Tests carried out at in imposed displacement rate of 0.2 μm/s (res. 20 μm/s) corresponds to a reference strain rate of 10−6s−1 (res. 10−4s−1)

6 Comparison between of cumulative strain fields between DIC results. (a) Experimental results at 600 °C, after 5 mm elongation at in imposed displacement rate of 0.2 μm/s. The sample thickness is 1 mm. (b) FE simulations results in the centre of the intrados of the V, at 600 and 650 °C, after 5  mm elongation at in imposed displacement rate of 0.2 μm/s

(6)

7 Diagram showing the results obtained for crack initiations on carbides or carbonitrides. Metallographic analysis of the material showed an average of 134 particles (carbides or carbonitrides) per mm2 with very large heterogeneities

8 Diagram showing the results obtained for intergranular crack initiations as a function of the strain rate in the centre of the area where SEM observations were performed

9 Diagram showing the results obtained for intergranular crack initiations for the slowest reference strain rate (10−6s−1

corresponding to an imposed displacement rate of 0.2 μm/s). Results are plotted as a function of the maximum cumulative strain in the center of the area where SEM observations were performed

(7)

67'DSSHDUVWREHDQLQKLELWLRQRILQWHUJUDQXODUFUDFNLQJ ,WLVNQRZQWKDWR[LGDWLRQRIQLFNHOEDVHGVXSHUDOOR\LQGXFHV YDFDQF\LQMHFWLRQLQWKHDOOR\15 7KHVHYDFDQFLHVFKDQJHGLIIX-VLRQNLQHWLFVRIVXEVWLWXWLRQDODWRPVDQGLQÀXHQFHGLVORFDWLRQ PRELOLW\22 due to coupling effects between plasticity and R[LGDWLRQ)XUWKHUPRUHVXFKLQWHUDFWLRQVEHWZHHQGLVORFD-WLRQVDQGVROXWHVSHFLHVDUHNQRZQWRRFFXUGXULQJG\QDPLF VWUDLQDJHLQJ '6$ DQG3RUWHYLQ/H&KkWHOLHU 3/& UHJLPHV )RU67'VRPHDXWKRUV OLQNWKLVVSHFL¿FLQWHU-JUDQXODUFUDFNLQLWLDWLRQWR'6$7KHJUDLQERXQGDULHVRI '$  DUH NQRZQ WR EH ZHDNHU WKDQ WKRVH RI 67'  /RFDOFKHPLFDOFRPSRVLWLRQLQÀXHQFHVSODVWLFGHIRUPDWLRQ DQGIDLOXUHPRGH1720GXHWRWKHUROHRILQWHUVWLWLDODWRPVVXFK DVFDUERQR[\JHQDQGQLWURJHQ([SHULPHQWDOO\LWLVIRXQG WKDWLIRQHORZHUVWKHDPRXQWRIFDUERQLQWHUVWLWLDOVLWDOVR GHFUHDVHV LQWHUJUDQXODU FUDFN LQLWLDWLRQ DW  ƒ& ,Q WKH FDVHRI'$JUDLQERXQGDULHVDUHHPEULWWOHGE\QDQR GHOWDSKDVHSUHFLSLWDWHVDQGWKHUHLVDJUHDWKHWHURJHQHLW\RI PHFKDQLFDOEHKDYLRXUEHWZHHQWKLVįSKDVHDQGWKHPDWUL[ LQWKH3)=7KLVPD\FRQWULEXWHWRVWUHVVFRQFHQWUDWLRQGXU-LQJWHQVLOHWHVWV$FFRUGLQJWRSUHYLRXVVWXGLHV15R[LGDWLRQ VRIWHQVDQGFKDQJHVWKHPDWHULDOPLFURVWUXFWXUHQHDUE\WKH VXUIDFHGXHWRFKURPLXPGHSOHWLRQ(DVLHUGLVORFDWLRQPRWLRQ DVVRFLDWHGZLWKYDFDQF\LQMHFWLRQGXHWRR[LGDWLRQPD\UHOD[ ORFDOVWUHVVFRQFHQWUDWLRQV7KHUHIRUHWKHVHSKHQRPHQDPD\ H[SODLQZK\ZLWKWKLVVSHFL¿FPLFURVWUXFWXUHR[LGDWLRQZDV IRXQGWRLQKLELWLQWHUJUDQXODUFUDFNLQLWLDWLRQ

Conclusion

7KHREMHFWLYHRIWKHSUHVHQWVWXG\ZDVWRLQYHVWLJDWHPHFKD- QLVPVIRULQWHUJUDQXODUFUDFNLQLWLDWLRQREWDLQHGGXULQJWHQ-VLOHWHVWVSHUIRUPHGDWDQGƒ&IRU'$DQGDW FXPXODWLYH SODVWLF VWUDLQ YDOXHV EHORZ  'HSHQGLQJ RQ WKHWHVWFRQGLWLRQVWKHIDLOXUHPHFKDQLVPPD\FKDQJHGUDVWL-FDOO\IURPFUDFNLQLWLDWLRQORFDWHGRQFDUELGHVWRLQWHUJUDQXODU GDPDJHLIVXI¿FLHQWSODVWLFVWUDLQ PRUHWKDQ LVFXPX-lated at a slow strain rate (10í sí 7KLVLQWHUJUDQXODUGDPDJH GHYHORSPHQWDOVRUHTXLUHVVSHFL¿FVWUHVVFRQGLWLRQVDVQR RFFXUUHQFHZDVREVHUYHGIRUVWUHVVWULD[LDOLW\RIEXWZDV REVHUYHGIRU)XUWKHUPRUHR[LGDWLRQVHHPVWRLQKLELWWKLV LQWHUJUDQXODUFUDFNLQLWLDWLRQ7KHVHUHVXOWVGLIIHUIURPWKRVH REWDLQHGIRU67'XQGHUWKHVDPHFRQGLWLRQV,WLVK\SRWK-HVLVHGWKDWWKHUROHRIWKHXQLTXHORFDOPLFURVWUXFWXUHDWWKH JUDLQERXQGDU\LQWKH'$PD\H[SODLQWKHVHUHVXOWVDUH LQLWLDWLRQZDVREVHUYHGIRUFXPXODWLYHSODVWLFVWUDLQ7KH PDLQGLIIHUHQFHEHWZHHQWKHWZRVDPSOHJHRPHWULHVLVWKH VWUHVVWULD[LDOLW\ZKLFKLVODUJHU DSSUR[LPDWHO\ IRUD 9VKDSHGVSHFLPHQLQVWHDGRIIRUDVWDQGDUGWHQVLOHVSHF-LPHQ)XUWKHUPRUHLQD9VKDSHVSHFLPHQVXUIDFHVWUHVVLV SURPRWHG&RPELQHGZLWKVSHFL¿FORDGLQJFRQGLWLRQV SODVWLF VWUDLQFXPXODWHGDWDVORZVWUDLQUDWH WKHVHWHVWLQJFRQGLWLRQV DSSHDUVWRFKDQJHWKHFUDFNLQLWLDWLRQEHKDYLRXU

Crack initiation due to carbide or carbonitride is widely rep RUWHG89 especially for fatigue tests on DA 718 alloys. Strain UDWHLVDSULPHRUGHUSDUDPHWHU7HVWVKLJKOLJKWDWKUHVKROG between 10í sí and 10í sí DQGWKHLQGHSHQGHQFHRIHQYL-URQPHQWFRQGLWLRQVKDVEHHQREVHUYHG7KHVHUHVXOWVFRXOG EHH[SODLQHGE\VSHFL¿FLWLHVRI'$7KHPLFURVWUXFWXUH RIWKHJUDLQERXQGDULHVLQ'$VLJQL¿FDQWO\GLIIHUVIURP WKHRQHLQ67'7KHSUHVHQFHRIįSKDVHDQGRIDSUHFLS-LWDWHIUHH]RQH )LJ2 DURXQG*%PXVWEHWDNHQLQWRDFFRXQW ZKHQRQHLVGHDOLQJZLWKLQWHUJUDQXODUIUDFWXUH

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ȝP&URVVVHFWLRQVFRQGXFWHGRQXQFUDFNHGJUDLQERXQG-DULHVUHYHDOHGQRR[\JHQHQULFKPHQW+RZHYHUDVRQO\VL[ FUDFNVZHUHLQYHVWLJDWHGQRVWDWLVWLFVRQWKHGHSWKRIWKHFUDFNV DUHDYDLODEOH2EVHUYDWLRQVDWWKLVVFDOHGRQRWDOORZVHHLQJ WKHFKDQJHVLQWKH3)=2QO\7(0FKDUDFWHUL]DWLRQVDWODUJHU PDJQL¿FDWLRQVFDQUHYHDOWKHFKDQJHVLQWKHPLFURVWUXFWXUHDQG HYHQFKHPLFDOFRPSRVLWLRQFKDQJHVLQ3)=GXHWRR[LGDWLRQ %XWXQIRUWXQDWHO\LQWKLVVWXG\WKHWKLQVHFWLRQSUHSDUDWLRQ IRU0(7KDVQRW\HWEHHQSRVVLEOHQHDUE\LQWHUJUDQXODUFUDFN 7KHVHQVLWLYLW\WRLQWHUJUDQXODUFUDFNLQLWLDWLRQRIFRQYHQ-WLRQDOO\KHDWWUHDWHG67'FDQEHFRPSDUHGZLWKWKDWRI '$DVUHVXOWVDUHDYDLODEOHLQWKHOLWHUDWXUH172024 for tests FRQGXFWHGXVLQJWKHVDPHFRQGLWLRQV7KHUHVXOWVIRU'$ GLIIHUIURPWKRVHREWDLQHGIRUWKH67'7KHHIIHFWRIJUDLQ ERXQGDU\ SUHFLSLWDWLRQ RQ WKH HQYLURQPHQWDO EHKDYLRXU RI

10 Diagram showing the results obtained for intergranular crack initiations for a 5  mm elongation (corresponding to 7% of cumulative strain in the centre of the V), for the slowest reference strain rate (10−6s−1 corresponding to an imposed

displacement rate of 0.2 μm/s). Results are plotted as a function of experimental conditions. Tests are performed under air or vacuum, with or without 8 h of pre-oxidation at the test temperature

(8)

6 'H\EHU )$OH[DQGUH - 9DLVVDXG DQG$ 3LQHDX µ3UREDELOLVWLF OLIH RI '$  IRU DLUFUDIW HQJLQH GLVNV¶ LQ µ6XSHUDOOR\   DQGYDULRXV'HULYDWLYHV¶(G($/RULD±2005706

3LWWVEXUJK3$86$

'/3UDNDVK0-:DOVK'0DFODFKODQDQG$0.RUVXQVN\µ&UDFN JURZWK PLFURPHFKDQLVPV LQ WKH ,1 DOOR\ XQGHU WKH FRPELQHG LQÀXHQFH RI IDWLJXH FUHHS DQG R[LGDWLRQ¶ Int. J. Fatigue2009 31

± ± ''.UXHJHUµ7KHGHYHORSPHQWRIGLUHFWDJHIRUJDVWXUELQHDJLQJ GLVNDSSOLFDWLRQ¶LQµ6XSHUDOOR\±0HWDOOXUJ\DQG$SSOLFDWLRQ¶(G ($/RULD±1989706:DUUHQGDOH3$86$ ( $QGULHX + *KRQHP $ 3LQHDX µ7ZR VWDJH FUDFN WLS R[LGDWLRQ PHFKDQLVPLQDOOR\60DOO¶LQµ(OHYDWHGWHPSHUDWXUHFUDFNJURZWK¶ (G71LFKRODV±1990$PHULFDQ6RFLHW\RI0HFKDQLFDO(QJLQHHUV 1HZ<RUN +*KRQHPDQG'=KHQJµ'HSWKRILQWHUJUDQXODUR[\JHQGLIIXVLRQGXULQJ HQYLURQPHQWGHSHQGHQWIDWLJXHFUDFNJURZWKLQDOOR\¶Mater. Sci. Eng. A1992150  ± ($QGULHX50ROLQV+*KRQHPDQG$3LQHDXµ,QWHUJUDQXODUFUDFN WLSR[LGDWLRQPHFKDQLVPLQDQLFNHOEDVHGVXSHUDOOR\¶Mater. Sci. Eng.

A1992154  ±

/)RXUQLHU''HODIRVVHDQG70DJQLQµ2[LGDWLRQLQGXFHGLQWHUJUDQXODU FUDFNLQJDQG3RUWHYLQ±/H&KDWHOLHUHIIHFWLQQLFNHOEDVHVXSHUDOOR\¶

Mater. Sci. Eng. A2001316 ± ±

%7HU2YDQHVVLDQ'3RTXLOORQ-0&ORXpDQG($QGULHXµ,QÀXHQFH RIORFDOPHFKDQLFDOORDGLQJSDWKVRQWKHR[LGDWLRQDVVLVWHGFUDFNLQLWLDWLRQ of alloy 718’. Mater. Sci. Eng. A2012533±

17RWVXNDDQG=6]NODUVND6PLDORZVNDµ(IIHFWRIHOHFWURGHSRWHQWLDO RQWKHK\GURJHQLQGXFHG,*6&&RIDOOR\LQDQDTXHRXVVROXWLRQDW ƒ&¶Corrosion198743  ± 17RWVXND(/XQDUVND*&UDJQROLQRDQG=6]NODUVND6PLDORZVND µ(IIHFWRIK\GURJHQRQWKHLQWHUJUDQXODUVWUHVVFRUURVLRQFUDFNLQJRIDOOR\ LQKLJKWHPSHUDWXUHDTXHRXVHQYLURQPHQWV¶Corrosion198743  ±

- 'HOHXPH ' 3RTXLOORQ 9 *DUDW - 0 &ORXp DQG ( $QGULHX µ0HFKDQLFDO EHKDYLRXU RI 6657 VSHFLPHQV RSWLPL]HG IRU ,*6&& concerns’. Corros. Sci.200850  ±

=HEXORQKWWSZZZQZQXPHULFVFRP.

3 * 0F&RUPLJN µ$ PRGHO IRU WKH 3RUWHYLQ/H &KDWHOLHU HIIHFW LQ substitutional alloys’. Acta Metallurgica197220  ±

3 :\FOLIIH µ'\QDPLF DQG VWDWLF VWUDLQ DJLQJ LQ VXEVWLWXWLRQDO DQG LQWHUVWLWLDO DOOR\V¶ LQ µ706 FRQIHUHQFH 3DSHU 6HOHFWLRQ  &21)  ¶1980. 9*DUDW-0&ORXH'3RTXLOORQDQG($QGULHXµ,QÀXHQFHRI3RUWHYLQ± /H&KDWHOLHUHIIHFWRQUXSWXUHPRGHRIDOOR\VSHFLPHQV¶J. Nucl. Mater.2008375  ± %0D[%9LJXLHU($QGULHXDQG-0&ORXHµ$5HH[DPLQDWLRQRIWKH 3RUWHYLQ/H&KDWHOLHU(IIHFWLQ$OOR\LQ&RQQHFWLRQZLWK2[LGDWLRQ Assisted Intergranular Cracking’. Metall. Mater. Trans. A201445  

± LQDFFRUGDQFHZLWKGLVFXVVLRQVRIPLFURPHFKDQLVPVIRXQG LQWKHOLWHUDWXUH+RZHYHUIXUWKHU7(0LQYHVWLJDWLRQVDUH UHTXLUHGWRXQGHUVWDQGFKDQJHVLQWKHPLFURVWUXFWXUHRUORFDO FKHPLFDOFRPSRVLWLRQDURXQGJUDLQERXQGDULHV

Acknowledgments

7KHDXWKRUVZRXOGOLNHWRWKDQN5RQDQ0DLQJX\DQG-HDQ &ODXGH6DODEXUDIRUWKHLUDVVLVWDQFHRQWHVWGHYLFHV0DULH &KULVWLQH/DIRQWIRU7(0REVHUYDWLRQV&ODXGLH-RVVHDQG 7HUHVD+XQJULD 806&DVWDLQJ IRU),%FKDUDFWHUL]DWLRQV

ORCID

D. Poquillon KWWSRUFLGRUJ

References

 ')RXUQLHUDQG$3LQHDXµ/RZF\FOHIDWLJXHEHKDYLRURILQFRQHODW .DQG.¶Metall. Trans. A19778  ±

 ++6PLWKDQG'-0LFKHOµ(IIHFWRIHQYLURQPHQWRQIDWLJXHFUDFN SURSDJDWLRQEHKDYLRURIDOOR\DWHOHYDWHGWHPSHUDWXUHV¶Metall. Mater.

Trans. A17  ±

 50ROLQV*+RFKVWHWWHU-&&KDVVDLJQHDQG($QGULHXµ2[LGDWLRQ HIIHFWV RQ WKH IDWLJXH FUDFN JURZWK EHKDYLRXU RI DOOR\  DW KLJK WHPSHUDWXUH¶Acta Materialia199745  ±

 -:DUUHQDQG'<:HLµ7KHF\FOLFIDWLJXHEHKDYLRURIGLUHFWDJHDW DQGƒ&¶Mater. Sci. Eng. A428 ± ±  36KDKLQLDQDQG.6DGDQDQGDµ&UDFNJURZWKEHKDYLRUXQGHUFUHHS IDWLJXHFRQGLWLRQVLQ$OOR\ LQQLFNHOFKURPLXPVWDLQOHVVVWHHO ¶LQ µ6\PSRVLXPRQ&UHHS)DWLJXH,QWHUDFWLRQ¶±1HZ<RUN  $'LERLQHDQG$3LQHDXµ&UHHSFUDFNLQLWLDWLRQDQGJURZWKLQ,QFRQHO

DOOR\DWƒ&¶Fatigue Fract. Eng. Mater. Struct.198710  

141–151.

 05:LQVWRQH.01LNELQDQG*$:HEVWHUµ0RGHVRIIDLOXUHXQGHU FUHHSIDWLJXHORDGLQJRIDQLFNHOEDVHGVXSHUDOOR\¶J. Mater. Sci.1985

20  ±

 - 3U\E\ORZVNL DQG 5 %DOOLQJHU µ,QÀXHQFH RI 0LFURVWUXFWXUH RQ WKH (QYLURQPHQWDOO\$VVLVWHG &UDFNLQJ RI ,QFRQHO ¶ Corrosion1987

43  ±

 ( $QGULHX 5 &R]DU DQG $ 3LQHDX µ(IIHFW RI HQYLURQPHQW DQG PLFURVWUXFWXUH RQ WKH KLJK WHPSHUDWXUH EHKDYLRU RI DOOR\ ¶ LQ µ6XSHUDOOR\±0HWDOOXUJ\DQG$SSOLFDWLRQV¶(G($/RULD±

Figure

Table 1  Chemical composition of 718 alloy (weight %)

Références